Tag Archives: all-Fe

First results on MgCl2 concentration in all-Fe WiSe flow batteries

In our previous post we described the research we will be doing on all-Fe flow batteries using water-in-salt (WiSe) electrolytes, thanks to the grant from NLnet. One of the first questions in that list was how the concentration of the WiSe salt affects the efficiency and stability of these batteries. Today I want to share the first set of results on this question, where we look at MgCl2 at different concentrations while keeping everything else in the battery the same.

For these experiments we used 1M FeCl2 (prepared from FeCl2.2H2O) and changed the MgCl2concentration from 3M up to 6M, with a 4.5M experiment in the middle. All the batteries were cycled at 10mA/cm2 using the same pump speed, charged to 20% of their total SOC and then discharged down to 0V. The actual electrolyte volumes ended up being different between experiments (from 9mL down to only 6mL for the 6M solution), so comparing capacities in mAh would be misleading. For this reason all capacities in this post are normalized by volume and reported in Ah/L. With this normalization the charge capacity is 2.68Ah/L in all cases, which makes the comparison a lot easier.

Voltage vs time for 1M FeCl2 with MgCl2 from 3M up to 6M, cycled at 10mA/cm2.

The graph above already shows that the batteries behave quite differently even though they start from very similar places. The first cycle had a low CE in all cases (86-90%), which is something I have seen before with these systems and is basically a conditioning effect of the electrolyte as the Fe chloride is partially oxidized (as it oxidizes slowly in air as a solid) and some electrons during the first cycle are just wasted reducing this Fe. After that, things start to diverge.

Efficiency values vs time for each MgCl2 concentration.

The 3M MgCl2 battery was the most stable one by far. Its CE was a bit erratic during the first 10 hours (one cycle dropped all the way to 84%) but then it settled at around 96% and stayed there for the whole 47 hours of cycling. The EE did start to go down after around 25 hours, ending at 63.7% after peaking close to 69%, but this decline was very slow compared to what we saw in the other two batteries. If we fit a line to the data the EE goes down by only 0.02% per hour.

The 4.5M battery actually gave the highest CE values of the series, between 97% and 98.6% for most of the test. With that said, the EE went from about 67% down to 57% in 42 hours, and since the CE barely moved, pretty much all of that loss comes from the voltage efficiency. There is also a jump at around 20-25 hours that is visible in all the graphs, and the discharge curve of cycle 10 shows some spikes. These were caused by a pump failure we had during this experiment, which interrupted the flow of electrolyte through the cell, so I wouldn’t read too much into that part of the data.

Discharge capacity in Ah/L and capacity retention relative to cycle 2.

The 6M battery is where things went clearly wrong. The CE started lower, at about 92%, and then fell sharply between 17 and 21 hours to around 85%. It never recovered after this. The discharge capacity dropped at exactly the same time, from 2.47Ah/L to 2.27Ah/L, which is a loss of about 8%. The EE ended at 52.6%, the lowest of the whole series, and it was declining at around 0.5% per hour, more than 20 times faster than the 3M battery. This battery also ran for the shortest time, because we had to stop the experiment after around 30 hours when the electrolyte started leaking. The leak was caused by clogging from Fe oxides that built up on the anolyte side, so by the end the battery was in quite bad shape.

Average charge and discharge voltages vs time, along with the voltage gap between them.

The voltage graphs help us understand where the EE losses are coming from. The gap between the average charge and discharge voltages grew in every battery, but in the 3M one it only went from 0.35V to 0.42V over 47 hours. For the 4.5M and 6M batteries the gap reached around 0.5V in 30-40 hours. The end of charge voltage of the 6M battery reached 1.40V after only 30 hours of cycling, and it was still going up when the experiment ended.

Charge and discharge curves early and late in each test, with capacity normalized by electrolyte volume.

Why would more MgCl2 make things worse? Concentrated MgCl2 solutions are quite viscous and their conductivity goes down as you add more salt, so I expected higher overpotentials at 6M from the start. What surprised me a bit is that the initial overpotentials were actually very similar, and the difference comes from how fast they grow. This suggests that something is building up in the cell over time, and in the 6M case we know at least part of the answer. The Fe oxides that clogged the anolyte side would also cover the electrode and make it harder for the electrolyte to flow through it, which fits nicely with the growing overpotentials. I believe the sudden drop in CE and capacity at 17-21 hours is the point where this clogging started to really affect the battery. Why the oxides built up so badly at 6M is something I don’t have a good answer for yet, and it is one of the things we will try to figure out with more cycling experiments.

Long story short, adding more MgCl2 does NOT make for a better all-Fe battery. The 4.5M electrolyte gives a slightly better CE, but the 3M electrolyte keeps its efficiency and capacity for a lot longer, which is what really matters in a flow battery. The next step will be to run the same comparison using CaCl2, and to do some longer tests at 3M to see where the slow EE decline ends up. The raw cycling data for these experiments will be released together with the rest of this first batch of results.

Thanks to NLnet for supporting this research!

Studying a WiSE based all-Fe chemistry using our flow battery kit

All-Fe flow batteries are very promising due to iron’s high abundance, low toxicity and low cost. In these batteries, FeCl2 is used as the main active salt in solution. When charging Fe2+ gets reduced to Fe metal on the anode while Fe2+ gets oxidized to Fe3+ on the cathode. However, these batteries suffer from a fundamental problem that has made their large scale adoption very difficult up until now.

Cyclic voltammetry of 1M FeCl2 and 4.5M CaCl2 using an Ag/AgCl reference electrode and a glassy carbon working electrode.

The main limiting problem of these batteries is H2 evolution at the anode. Since Fe plating happens at a lower potential than H2 evolution, there is always some hydrogen generation when the battery is charged. This H2 evolution causes an increase in the pH of the battery which then causes iron hydroxides and oxides to precipitate out of solution. This causes passivation of Fe metal surfaces, loss of capacity and potentially clogging of the battery.

A few years ago, Tao Gao’s group in Utah discovered that CaCl2 and MgCl2 water-in-salt-electrolytes (WiSE) (read the paper here) could substantially improve Fe plating behavior. While they didn’t test this in flow batteries, they showed that very high Coulomb efficiencies with very low hydrogen evolution rates were possible when using these salts. This is because these salts bond with water and therefore make it substantially harder for water to get reduced at the anode. We are talking about very highly concentrated solutions though, around 4.5M CaCl2, which is around 660g/L of CaCl2.2H2O.

Plate/strip experiment using the 1M FeCl2, 4.5M CaCl2 electrolyte.

We recently obtained some of these reagents to test these chemistries in our flow battery kit. I first ran CV experiments of the 4.5M CaCl2 electrolyte with 1M FeCl2 and obtained the curves showed above. This reveals standard potentials of -0.71V and 0.55V for the two half reactions, which means our battery should have a max potential of around 1.26V. I then ran plate/strip experiments (using different plating times), which generated the second curve above. Using the slope of this plot we can extract the plating efficiency, which is >99% in this case. This means that very little hydrogen evolution is happening within this electrolyte, a result I had never seen with FeCl2 solutions and which is in agreement with the Tao Gao group paper.

After doing this I then ran a flow battery using this electrolyte and noticed some problems with capacity loss because of undissolved metallic Fe on the anode using a Daramic separator. It seems that the above electrolyte has some issues with the reversibility of the plating reaction. While little hydrogen is generated on plating, there still seem to be some important losses of capacity due to passivation of the Fe. To fix this problem I then added 1M NH4Cl into the electrolyte, which helped me fix this issue when dealing with Zn-I flow batteries.

Cycling of an all-Fe battery using 1M FeCl2, 4.5M CaCl2 and 1M NH4Cl. Cycling was done at 20mA/cm2 Charging was done to 4Ah/L and discharge was done to 0V.

I cycled the battery at 4Ah/L, which generated the results above. You can see that we get extremely good CE values (97.88%) which are even better than those we were obtaining with the Zn-I system, even though we’re using a microporous separator. The energy efficiency is lower than for Zn-I but still reaches a value of 53.27%. Given a concentration of 1M FeCl2 , 4Ah/L represents a state-of-charge (SOC) of ~30%. The cycling is stable, although some increase of the charging voltage is indeed happening through time (although this is also matched by an increase in the discharge voltage). The mean discharge potential is quite low though, at 0.7V, which means we have considerable ohmic losses at this current density.

I am now testing the electrolyte at higher SOC values and will continue testing MgCl2 and other modifications, such as additions of ascorbic acid and thiosulfate to remove oxygen from the initial solutions and improve the initial state of the battery (as some capacity is lost due to the presence of oxidized Fe in the initial solution). Make sure to follow our progress on this forum thread.

This flow battery kit work is being funded by the Financed by Nlnet’s NGI0 Entrust Fund. We are also collaborating with the FAIR Battery project.